QA: Keeping Print Layer Lines off the Casting

问答:3D 打印母版的层纹怎么不带到铸件上

type:featured-qa · level:intermediate · material:bronze · variant:castable-resin · scale:decorative-object · equipment:hand-tools · stage:patternmaking

标签:层纹,二次固化,底漆,层厚,铸件表面

层纹带入铸件多因三点:层厚过大(应选 0.03 mm 以下)、二次固化过度导致翘曲、未喷底漆封闭。正确顺序:405 nm 固化至表面不再发黏(10–15 分钟,勿超 20 分钟),800 目水砂轻磨后喷 2 遍细底漆,干燥 2 小时再翻模。铸件表面只需轻抛即可消除残余台阶。

Layer lines usually come from excessive layer height (use 0.03 mm or finer), over-curing that warps the part, or skipping primer. Cure under 405 nm only until the surface is no longer tacky (10–15 min, never over 20), light-sand with 800-grit wet paper, spray two fine primer coats, and dry 2 h before moulding. A light polish on the final casting removes any residual steps.